性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | |
基本性能 | 吸水率 | ASTM D-570 | 0.04 | % | |
物理性能 | 比重 | ASTM D-792 | 1.39-1.43 | ||
玻璃纤维含量 | Ash | 15 | % | ||
成型收缩率 | ASTM D-955 | 0.2-1.4 | % | ||
机械性能 | IZOD冲击强度 | ASTM D-256 | 5-7 | Kg.cm/cm | |
洛氏硬度 | ASTM D-785 | 93 | M-Scale | ||
引张伸长率 | ASTM D-638 | 4-5 | % | ||
挠曲强度 | ASTM D-790 | 1300-1500 | Kg/cm2 | ||
挠曲弹性率 | ASTM D-790 | 40000-50000 | Kg/cm2 | ||
引张强度 | ASTM D-638 | 800-1000 | Kg/cm2 | ||
电气性能 | 表面电阻率 | ASTM D-257 | >1014 | Ω | |
诱电正接 | 60Hz | ASTM D-150 | 0.001 | ||
绝缘破坏强度 | ASTM D-149 | 20 | KV/mm | ||
体积电阻率 | ASTM D-257 | >1016 | Ω.cm | ||
诱电率 | 60Hz | ASTM D-150 | 3.3 | ||
耐电弧性 | ASTM D-495 | 129 | sec | ||
热性能 | 热变形温度 | 4.6Kg/cm2 | ASTM D-648 | 220 | ℃ |
线膨胀系数 | ASTM D-696 | 5 | 10-5cm/cm℃ | ||
熔点 | DSC | 225 | ℃ | ||
热变形温度 | 18.6Kg/cm2 | ASTM D-648 | 206 | ℃ | |
耐燃性 | 0.83mm | UL 94 | HB |
PBT性质:为高结晶性热可塑性塑料,熔点220~230℃,结晶速率比PET快。
PBT优点:机械性质安定抗张强度与抗张模数和尼龙相似、摩擦系数小有自润性、吸水率低、电气性质优良、尺寸安定性良好、耐药品性、耐油性极佳。缺 点:Tg(30℃)低,在荷重下H.D.T.为60℃、抗冲击强度不良,一般以玻纤补强为FR-PBT来使用.
PBT用 途:1)、电子电器:无熔线断电器、电磁开关、驰返变压器、家电把手、连接器、外壳. 2)、汽车: 车门把手、保险杆、分电盘盖、挡泥板、导线护壳、轮圈盖工业零件:OA风扇、键盘、钓具卷线器、零件、灯罩.
PBT 基础创新塑料(美国) SABIC Valox PBT(聚对苯二甲酸丁二醇脂):
Valox DR51M特性:15%玻璃纤维增强型PBT.机械/热/电气性能强; 阻燃.用于聚光灯,家电外壳和处理.易流动,易脱模.
PBT理化特性 : PBT为乳白色半透明到不透明、结晶型热塑性聚酯。具有高耐热性、韧性、耐疲劳性,自润滑、低摩擦系数,耐候性、吸水率低,仅为0.1%,在潮湿环境中仍保持各种物性(包括电性能),电绝缘性,但体积电阻、介电损耗大。耐热水、碱类、酸类、油类、但易受卤化烃侵蚀,耐水解性差,低温下可迅速结晶,成型性良好。缺点是缺口冲击强度低 ,成型收缩率大 。故大部分采用玻璃纤维增强或无机填充改性,其拉伸强度、弯曲强度可提高一倍以上,热变形温度也大幅提高。可以在140℃下长期工作,玻纤增强后制品纵、横向收缩率不一致,易使制品发生翘曲。